Contact us
- : 0086-371-86151627 0086-371-86151827
- : 0086-371-86011881
- : [email protected]
- : [email protected]
- : bebonchina
Products- Boiler steels
- High carbon steel
- High Yield steel
- steel for welded tubes
- General construction steel
- steel with Cr.,Mo.,Cr-Mo
- Steel for large diameter pipes
- Simple pressure vessels steel
- Steel for gas cylinders and gas vessels
- General purpose structural steels
- Steel for boilers and pressure vessels
- steel resistant to atmospherical corrosion
- Carbon steel and low alloy steel
- Fine-grain structural steels,normalised rolled
- weldable normalized fine grained pressure vessel steels
News- Paper Machine Thick Steel Plates for
- Sugar Mill Thick Steel Plates for Pr
- Tunnel Boring Machine Thick Steel Pl
- Railway Bogie Thick Steel Plates for
- Thick Steel Plates in Large Hydrauli
- Thick Steel Plates for Large Bulk Ma
- Heavy Machine-Bed Thick Steel Plates
- Penstock Thick Steel Plates for Hydr
- FPSO Hull Thick Steel Plates for Flo
- Building-Structural Thick Steel Plat
Methods to repair defects of A283GrC seamless steel pipe
When there are too many defects in the welded joints of A283GrC seamless steel pipes, welding repairs can be used for repairing. Note that the number of times of welding and repairing alloy steel at the same position is not more than 2 times, and the following regulations must be met:
1. Defects must be completely eliminated;
2. When welding A283GrC seamless steel pipes, corresponding measures need to be formulated and approved in strict accordance with the requirements of the repair process;
3. Re-appearance inspection and spectral analysis are required after rework;
4. Then heat-treat the joints of A283GrC seamless steel pipes;
5. The repair service should carry out the necessary hardness test after the heat treatment of the A283GrC seamless steel pipe;
6. After heat treatment, the reworked joint must be consistent with the original process flaw detection again.